China 45-Permalloy Soft Magnetic Alloy Wire Ni46, Find details about China Soft Magnetic Alloy Wire, Ni46 from 45-Permalloy Soft Magnetic Alloy Wire Ni46
composition | C | P | S | Mn | Si |
≤ | |||||
Content(%) | 0.03 | 0.02 | 0.02 | 0.6~1.0 | 0.15~0.3 |
composition | Ni | Cr | Mo | Cu | Fe |
Content(%) | 45.0~46.5 | - | - | 0.2 | Bal |
Shop sign | Melting point (ºC) | Resistivity (μΩ·m) | Density (g/cm³) | Curie point (ºC) | Saturation magnetostriction coefficient (10-6) |
1j46 | 10.9~11.2 | 0.56 | 8.75 | 400 | 0.5 |
shop sign | Annealing medium | heating temperature | Keep the temperature time/h | Cooling rate |
1j46 | Dry hydrogen or vacuum, pressure is not greater than 0.1 Pa | Along with the furnace heating up 1100~1200ºC | 3~6 | In 100 ~ 200 ºC / h speed cooling to 600 ºC, fast to 300 ºC draw a charge |