China Glass Sealing52 Tube Used in Multipin Headers for Relays, Coils and Capacitors, Find details about China Alloy52 Tube, 52h Capillary Tube from Glass Sealing52 Tube Used in Multipin Headers for Relays, Coils and Capacitors
Ni | 51.5~52.5 | Fe | Bal. | Co | - | Si | ≤0.3 |
Mo | - | Cu | - | Cr | - | Mn | ≤0.8 |
C | ≤0.05 | P | ≤0.02 | S | ≤0.02 |
Density (g/cm3) | 8.25 |
Electrical resistivity at 20ºC(ohm.mm2/m) | 0.43 |
Temperature factor of resistivity(20ºC~200ºC)X10-6/ºC | 9.8~11 |
Thermal conductivity, λ/ W/(m*ºC) | 16.7 |
Curie point Tc/ ºC | 520 |
Elastic Modulus, E/ Gpa | 144 |
θ/ºC | α1/10-6ºC-1 | θ/ºC | α1/10-6ºC-1 |
20~-60 | 20~100 | 10.3 | |
20~-40 | 20~200 | 10.4 | |
20~-20 | 20~300 | 10.2 | |
20~-0 | 20~350 | 10.3 | |
20~50 | 20~400 | 10.3 | |
20~100 | 20~450 | 10.3 | |
20~150 | 20~500 | 10.3 | |
20~200 | 20~600 | 10.8 |
Tensile Strength | Elongation |
Mpa | % |
641 | 14 |
689 | 9 |
731 | 8 |
The heat treatment process | |
Annealing for stress relief | Heated to 530~550ºC and hold 1~2 h. Cold down |
annealing | In order to eliminate hardening, which be bring out in cold-rolled, cold drawing process. Annealing needs heated to 830~880ºC in vacuum,hold 30 min. |
The stabilization process | In protective media and heated to 830 ºC, hold 20min. ~ 1h, quench Due to the stress generated by quenching, heated to 315ºC,hold 1~4h. |
Precautions | Can not be hardened by heat treatment, Surface treatment can be sandblasting, polishing or pickling. Alloy can be used 25% hydrochloric acid pickling solution at 70 ºC to clear oxidized surface |