S B R | 1 5 0 0 | ||||||
PRODUCT DESCRIPTION (SBR1500 VER. M _ ASTM) | DATE: 16 NOV. 97 | ||||||
COLD MIXED SOAP STYRENE BUTADIENE COPOLYMER, 23.5 % BOUND STYRENE, WITH A STAINING ANTIOXIDANT. | |||||||
RAW POLYMER PROPERTIES | |||||||
MOONEY VISCOSITY (PTS) | METHOD (**) | ||||||
(ML 1+4 AT 100 0C) | 50 +/- 6 | ASTM D 1646-96A | |||||
VOLATILE (WT %) | 0,4 MAX. | ASTM D 1416 | |||||
ASH (WT %) | 0,6 MAX. | ASTM D 1416 | |||||
ANTIOXIDANT (WT %) | 1.00 - 1.40 | ASTM D 1416 | |||||
SPECIFIC GRAVITY | 0,92 | ||||||
BOUND STYRENE (WT %) | 22.5 - 24.5 | ASTM D 1416 | |||||
FREE ORGANIC ACIDS (WT %) | 5.00 - 6.50 | ASTM D 1416 | |||||
ORGANIC ACIDS SOAPS (WT %), MAX. | 0.20 | ASTM D 1416 | |||||
IRON CONTENT (WT %), MAX. | 0.005 | ASTM D 1416 | |||||
COPPER CONTENT (WT %), MAX. | 0.0002 | ASTM D 1416 | |||||
RHEOMETRIC PROPERTIES (1) | |||||||
MAXIMUM TORQUE, MH (IN/LB.) | 38 +/- 5 | ASTM 2084 | |||||
TORQUE ML (IN/LB.) | 8 +/- 1.5 | ASTM 2084 | |||||
T-90 M: S (1) | 15:10 +/- 3.5 | ASTM 2084 | |||||
COMPOUNDED AND OTHER TYPICAL PROPERTIES | |||||||
MODULUS AT 300 % ELONGATION, (KGF/CM2)*, 35 MIN CURED | 130 | ASTM D 412 | |||||
ULTIMATE TENSILE STRENGTH, (KGF/CM2) *, 35 MIN CURED | 230 | ASTM D 412 | |||||
ULTIMATE ELONGATION, (%), 35 MIN CURED | 470 | ASTM D 412 | |||||
PACKAGING | |||||||
BALE WEIGHT, (KG) | 30 +/- 1 | ||||||
FILM WRAP | 50MKM +/- 5 | ||||||
VICAT POINT, (DEG C) | 110 | ||||||
PALLET WEIGHT, (KG) | ABOUT 450 |
SBR 1500 | 100 | RHEOMETER CONDITIONS |
DG-100 CHANNEL BLACK | 50 | 160OC, 1 ARC, 100 CPM, MICRO DIE. |
ZINC OXIDE | 3 | |
STEARIC ACID | 1 | |
2,2'-BENZOTHIAZOLYL DISULFIDE | 3 | |
SULFUR | 1.75 |